Delrin vs Nylon: Which Plastic for Your Part?
Delrin (acetal) and nylon 6/6 are two of the most common plastics for machined parts, and choosing between them is the most common material question we get. Here they are side by side, from the datasheets for the stock shapes parts are cut from, with what the difference means on the machine and in service.
The short answer
Toughness in service, or dimensional stability: that trade-off usually settles it. Nylon takes up moisture, which makes it tougher and lets a machined part grow. Delrin barely does, which is why it holds a tight fit.
Choose Delrin when
- The part has to hold a tight fit, especially in humid or wet service.
- Precision gears, bushings and bearings that must keep their size.
- Low-friction wear surfaces that run without lubrication, or in wet wear.
- You want a fine machined finish and clean, predictable chips.
Choose nylon when
- The part takes shock loads: gears, sprockets and sheaves that run quietly against metal parts.
- Abrasion in dry service, where nylon wears better than acetal and forgives marginal lubrication.
- Large sections, such as a big gear or wear pad: cast nylon 6, a different grade from the nylon 6/6 in the table, is made in much larger cross-sections than extruded stock.
- Toughness in service matters more than holding a tight dimension.
Delrin vs nylon properties
Typical values, not a specification. Delrin: unfilled acetal homopolymer stock shapes (Ensinger TECAFORM AD, made from Delrin 150 series resin, and MCAM Acetron). Nylon: unfilled nylon 6/6 stock shapes, dry (MCAM Ertalon 66 SA / Nylatron 101, with Ensinger TECAMID 66 where noted). Each figure is the one on that material’s own page, with its datasheet linked.
| Property | Delrin | Nylon 6/6 | Test |
|---|---|---|---|
| Density | 1.41 g/cc | 1.15 g/cc | ASTM D792 |
| Tensile strength | 11,000 psi at yield | 12,000 psi at yield | ASTM D638 |
| Tensile modulus | 350,000 psi | 425,000 psi | ASTM D638 |
| Flexural modulus | 470,000 psi | 450,000 psi | ASTM D790 |
| Hardness | 94 Rockwell M | 85 Rockwell M | ASTM D785 |
| Izod impact, notched | 1.0 ft-lb/in | 0.6 ft-lb/in | ASTM D256 |
| Max continuous service temp | 180 °F | 185 °F Ensinger's long-term rating. MCAM's sheet prints 210 °F in its 20,000-hour row, against 80 °C (176 °F) in its own metric column. | Delrin: manufacturer rating (continuous, 20,000 h in air) Nylon 6/6: manufacturer rating (long term) |
| Heat deflection temp @ 264 psi | 250 °F | 194 °F | ASTM D648 |
| Water absorption, 24 h | 0.2 % | 0.3 % | ASTM D570 |
| Thermal expansion (CTE) | 6.8 ×10⁻⁵ in/in/°F | 5.5 ×10⁻⁵ in/in/°F | Delrin: ASTM D696 Nylon 6/6: ASTM E831 (TMA), -40 to 300 °F |
| FDA food contact | Yes, natural grade Applies to natural Delrin 150SA and Acetron POM-H stock under 21 CFR 177.2480. Black and filled grades are not covered. The linked brochure lists the grade as FDA compliant; the CFR section is from the k-mac Plastics and Ready Plastics grade pages. Confirm the grade on the mill cert. | Yes Under 21 CFR 177.1500. |
Figures are dry, as machined. Strength and stiffness fall as the part takes up moisture; impact resistance rises.
The two thermal expansion figures come from different test methods, so don’t read the gap between them as a real difference. For a critical fit, compare the two materials on one supplier’s datasheets.
What the numbers mean
Moisture: the difference that matters most
On the 24-hour test the two look close: 0.2% for Delrin, 0.3% for nylon 6/6. The 24-hour figure hides the real gap. Nylon keeps taking on water until it saturates at around 7 to 8%, and swells as it does, by roughly 2.5 to 3% in size at full saturation. Acetal absorbs roughly an eighth as much at saturation. For scale, a 100 °F temperature swing moves either material by well under 1% (about 0.7% for Delrin). Water also changes nylon’s properties: it gets tougher and takes impact better, and loses stiffness and tensile strength. The datasheet describes a dry part; your part may not stay dry.
Strength, hardness and impact
Dry, nylon 6/6 tests a little higher on tensile strength (12,000 against 11,000 psi, at yield). Delrin is harder (Rockwell M94 against M85). On notched impact, dry nylon actually tests lower than Delrin (0.6 against 1.0 ft-lb/in); nylon’s reputation for toughness is largely earned once it has taken up moisture.
Heat
Their continuous service ratings are close: 180 °F for Delrin and 185 °F for nylon 6/6. Under load Delrin keeps its stiffness to a higher temperature: its heat deflection temperature at 264 psi is 250 °F against 194 °F. If the part runs hotter than either, look at PEEK or Ultem. To see how far a part of either material moves over a temperature range, use the thermal expansion calculator.
Wear and friction
Both are bearing and wear materials. Nylon has better abrasion resistance than acetal in dry service and is forgiving of marginal lubrication. Acetal is rated better in wet wear, and runs on wear surfaces without lubrication.
Chemicals
Neither is the plastic for strong acids or strong oxidizers. Delrin, the homopolymer, is also attacked by strong bases, so caustics, and chlorinated sanitizers at use strength, are better handled by acetal copolymer. Nylon is also attacked by halogens.
Machining Delrin vs machining nylon
- Chips. Delrin makes clean, continuous chips and standard chip breakers usually work on it. Nylon makes long, stringy chips that wrap tooling and are hard to break, because it is so tough; plan on a pick-off, peck drilling and air to clear them.
- Spring-back. Nylon deflects away from the tool and relaxes back afterwards, so reamed holes tend to finish undersize and nylon is usually tapped slightly oversize. Delrin is one of the more dimensionally cooperative plastics on a mill or lathe.
- Coolant. Many Delrin jobs run dry with air or a light mist. Nylon generates more frictional heat and benefits from coolant more, but on tight work air or mist is safer than water-based flood, which can cost more in swell than it gains in heat.
- Tolerance. Machined-plastic tolerance is best thought of in proportion to size, roughly ±0.001″ per inch. On well-planned acetal setups we routinely hold ±0.002″. With nylon, moisture and spring-back, not the machine, set the limit, so tolerances should be set with the working environment in mind.
More detail in our Delrin machining guide and nylon machining guide, and on the Delrin and nylon 6/6 material pages.
Delrin vs nylon: common questions
- Is Delrin stronger than nylon?
- Not on tensile strength. Dry, as machined, nylon 6/6 stock tests at 12,000 psi at yield against 11,000 psi for Delrin. Delrin is harder, holds its stiffness to a higher temperature under load, and barely changes with humidity, while nylon loses strength and stiffness as it takes up moisture.
- Which holds tighter tolerances, Delrin or nylon?
- Delrin. It absorbs very little moisture, so a machined part keeps its size in service. Nylon takes on water and grows, and it springs back from the cutter, so reamed holes tend to finish undersize. On well-planned acetal setups we routinely hold ±0.002″, and tighter on selected critical features when the part is designed for it.
- Is acetal the same as Delrin?
- Delrin is a brand of acetal: the homopolymer (POM-H). The other common form is acetal copolymer (POM-C). Homopolymer is roughly 15% stronger and stiffer; copolymer handles hot water, caustics and thick sections better. Against nylon, both forms of acetal make the same trade: more dimensional stability, less toughness once nylon has taken up moisture.
- Which is better for gears and bushings?
- Both are used for them. Delrin is the choice for precision gears and bushings that must keep their size, and for wet service. Nylon is the choice for gears and sheaves that take shock loads, for dry abrasion, and for large parts machined from cast nylon 6.
- Can you machine both?
- Yes. We stock Delrin and nylon in sheet, rod and tube and machine both to print, from one-off prototypes through production runs. Send the drawing with the service environment and we will tell you which one will hold your fit.
Not sure which one your part needs?
Send the drawing with the service environment and we will tell you which plastic will hold your fit. Plastic machining in Linden, New Jersey since 1968.